Component dosage /g component dosage /g
Hydrochlorinated rubber 100 Sulfur
Accelerator 2.5 Dichloroethane 400
Preparation and curing    Weigh in order and mix well. Curing at 0.5MPa and 150 °C for 0.5h .
Use The glue is mainly used for the bonding of rubber and metal.